Ask ten suppliers which blade steel is more wear resistant and you will get ten versions of "very good". Nobody offers a number with a unit on it. Buyers end up comparing hardness instead, because HRC is the only figure on the certificate. It is also the wrong one for this question. Two tool steels can both read 60 HRC and lose very different amounts of metal when abrasive material slides across them. How much material a shear blade loses to abrasion is measured as volume loss in cubic millimetres in an ASTM G65 dry sand/rubber wheel test, and in one published series D2 at 60 HRC lost 41.0 mm³ while a high-vanadium powder-metallurgy steel at the same 60 HRC lost 11.1 mm³. Same hardness, 3.7 times the wear.
That gap is the reason astm g65 volume loss for tool steel blades is worth putting on an enquiry alongside HRC. It will not tell you how many tons a blade will cut — no laboratory test does — but it does separate grades that a hardness reading cannot. On a rotor full of shredder blade abrasive feed, that distinction tends to show up long before the hardness does.
Key Takeaways
- ASTM G65 reports volume lost, not a grade. Lower mm³ means better resistance to low-stress sliding abrasion.
- Same hardness, different wear: at 60 HRC, D2 lost 41.0 mm³ and Micro-Melt A11 lost 11.1 mm³ in the same test series.
- M2 at 65 HRC lost 23.3 mm³, about half of D2 at 60 — so hardness is not the only variable.
- G65 is a sand-and-rubber-wheel test. It ranks resistance to low-stress abrasion; it does not reproduce the high-load edge contact of a shear.
- Datasheet values are typical averages, not batch guarantees. Always state the procedure and load when you quote a number.
What Does a Volume-Loss Number Actually Measure?
A dry sand/rubber wheel test presses a steel coupon against a rotating rubber wheel while measured sand feeds between them. After a fixed run the coupon is weighed and its loss converted to cubic millimetres. Dry sand rubber wheel wear test results for D2 and A11 below come from one published comparison by Carpenter Technology, all ASTM G65 Method A, 30 minutes, all measured the same way. That common method is what makes the rows comparable:
| Alloy / condition | Hardness (HRC) | G65 volume loss (mm³) | Lower loss means |
|---|---|---|---|
| Micro-Melt A11 (PM) | 64.0 | 9.0 | Best in this series |
| Micro-Melt A11 (PM) | 60.0 | 11.1 | 3.7x better than D2 at the same HRC |
| Micro-Melt A11-LVC (PM) | 55.0 | 14.4 | Still ahead of D2, five HRC points softer |
| Micro-Melt A11-LVC (PM) | 49.0 | 16.3 | Carbide content still doing the work |
| AISI M2 | 65.0 | 23.3 | Around half the loss of D2 |
| AISI D2 / Cr12MoV | 60.0 | 41.0 | Common cold-shear baseline |
| AISI A2 | 60.0 | 62.6 | Tougher matrix, faster sand wear |
| AISI H13 | 51.0 | 127.0 | Hot-work steel, poor cold abrasion choice |
Read the table as a ranking of low-stress slurry and sand abrasion, not a blade-life forecast. An independent coating laboratory using the same procedure puts D2 at 36.1 mm³ and cemented tungsten carbide near 2.5–7 mm³, which sits close to the Carpenter figures and confirms the order of magnitude. Note the H13 row: a hot-work grade at 51 HRC lost more than three times what D2 lost and fourteen times what A11 lost. That is why H13 belongs in hot shear sections, not in a cold plate line. On a scrap shear blade wear grade decision, the grade and its carbide make-up matter more than one more point on the Rockwell scale.
Why Do Two Steels at 60 HRC Wear So Differently?
Because HRC measures how far a diamond indenter sinks in, while sand abrasion is thousands of tiny scratches. Resistance to the second depends on how many hard particles sit in the steel and how well the matrix holds them. Why two steels at the same hrc wear differently comes down to carbide type, carbide distribution and the temper condition. This is a qualitative comparison drawn from the same published series — no extra numbers are being invented here:
| What sits in the steel | D2 / A2 pattern | A11 / M2 pattern | Effect on the G65 result |
|---|---|---|---|
| Carbide family | Chromium carbides in D2, fewer in A2 | Fine vanadium-rich carbides, tungsten and molybdenum in M2 | Vanadium-rich carbides are harder than the sand and stay in the surface |
| Carbide distribution | Coarser carbides, more spacing between them | Fine, evenly spread particles in a powder-metallurgy structure | Sand has fewer soft paths to plough through |
| Matrix toughness | A2 gives up abrasion to gain shock tolerance | Higher alloy content carries more load at the same HRC | Wear rank and shock rank rarely agree |
| Where it applies on a blade | Clean plate, steady feed, predictable grade | Long runs on abrasive feed or filled material | Payback comes from uptime, not from the grade price |
The distinction that matters to a buyer: what g65 volume loss predicts about shear blade life is only the abrasive part of the job. A guillotine edge sees high contact stress, a thin wedge and occasional shock; a G65 coupon sees loose sand at moderate load. The test is good at answering "will this grade survive scale and slurry?" and poor at answering "will this edge chip on rebar?". Use it to shortlist grades, then confirm on the machine. For a briquetting die abrasion rate, the same warning applies in reverse: the die sees pressure and flow, not a rolling rubber wheel.
What Should You Write on an Abrasion Test Request?
A bare "41 mm³" is not a specification, because changing the procedure can change the number by several times without changing the steel. What to put on a blade abrasion test request is the set of conditions around the figure. Procedure A in the standard runs 6,000 revolutions over 30 minutes at 130 N load against a 60 Shore A wheel with dry sand fed at about 342 g/min — and every one of those fields belongs on the request:
| Field on the request | Wording that removes doubt | Why the mm³ moves |
|---|---|---|
| Procedure and load | "ASTM G65, Procedure A, 130 N" | A different procedure is a different test, not a better result |
| Duration | "6,000 revolutions / 30 min" | Short runs favour materials that work-harden |
| Abrasive feed | "Dry Ottawa sand, 342 g/min" | Sand lot and flow rate change the cutting action |
| Condition of the coupon | "Ground surface, state the hardness actually measured" | A decarburised skin wears away first |
| Result unit | "Volume loss in mm³, not mass loss in grams" | Densities differ; grams cannot rank grades |
| Status of the value | "Typical datasheet value or measured batch?" | Published figures are averages, not acceptance limits |
Those six fields are the whole of blade supplier wear test report requirements for a useful comparison. If a supplier quotes a lower number without naming the procedure, assume nothing: it may be a different test, a different load or a coating that will not survive your blade geometry. Ask for the grade, the measured HRC and the test conditions in the same sentence.
FAQ
What is a good ASTM G65 volume loss for a shear blade steel?
On the Method A series quoted above, roughly 9–23 mm³ is the high-wear end (PM A11, M2), 40–65 mm³ is the conventional cold-work band (D2, A2), and H13 sits near 127 mm³. There is no pass mark, because the right figure depends on how abrasive your feed is. Use the number to rank grades within one published test series, never as an acceptance limit on a purchase order.
Why is D2 so much worse than A11 when both are 60 HRC?
The indenter in a hardness test only sees the average resistance of the surface. Sand abrasion sees the gaps between carbides. D2's chromium carbides are coarser and more widely spaced than the fine vanadium-rich carbides in a powder-metallurgy A11, so loose grains find an easier path through D2. Same HRC, 41.0 mm³ against 11.1 mm³ in the same test.
Can I convert an ASTM G65 number into blade life in tons?
No. G65 is a low-stress abrasion test with loose sand and a rubber wheel; a blade edge carries high local load and may see shock, heat and adhesion as well as abrasion. A grade that wins the G65 ranking can still chip first on tramp metal. Track tons per edge on your own machine and use the laboratory number to choose which grades to try.
Why do some suppliers quote grams instead of cubic millimeters?
Mass loss is what the balance actually measures; ASTM G65 asks for it to be converted to volume loss. Grams are misleading when comparing unlike materials because density differs — a carbide and a steel can lose the same mass while losing very different volumes. Ask for mm³ and for the density used in the conversion.
Is a powder-metallurgy grade always worth the extra cost?
Only where abrasion dominates the failure. In the published series a PM A11 at 60 HRC lost about a quarter of D2's volume, which can pay for itself in long, abrasive runs where changeovers are expensive. On clean plate with occasional shock, toughness and edge geometry decide the outcome and D2 remains the economical choice. Match the grade to the failure you actually see.
Hardness tells you how a blade resists a dent. Impact energy tells you how it survives a blow. Compressive strength tells you when it stops holding its shape. Wear resistance specification beyond the hardness scale needs a fourth figure: volume lost under a named abrasion test. Put the grade, the measured HRC and the G65 conditions together, then compare like with like. Browse the blade range at GOOD-KNIFE and tell us what your shear actually cuts — the feed, the section and the failure you see — and we will suggest grades worth testing side by side.